利用镁合金快速定量测氢仪研究了通Ar除气对AZ91镁合金熔体除气处理的效果,以及通Ar流量、通Ar时间及精炼温度三因子对精炼效果的影响.运用正交试验方法找到了通Ar除气工艺的最佳工艺参数匹配,即通Ar流量为1~1.5L/min,通Ar时间为20~25min,镁液温度为725~750℃.揭示了主要工艺参数对镁合金熔体净化的影响规律.

参考文献

[1] Yuan Guangyin;Liu Manping;Ding Wenjiang .Microstructure and mechanical properties of Mg-Zn-Si-based alloys[J].Materials Science & Engineering, A. Structural Materials: Properties, Misrostructure and Processing,2003(1/2):314-320.
[2] Du WW.;Sun YS.;Min XG.;Xue F.;Zhu M.;Wu DY. .Microstructure and mechanical properties of Mg-Al based alloy with calcium and rare earth additions[J].Materials Science & Engineering, A. Structural Materials: Properties, Misrostructure and Processing,2003(1/2):1-7.
[3] Yuan Guangyin;Sun Yangshan;Ding Wenjiang .Effects of bismuth and antimony additions on the microstructure and mechanical properties of AZ91 magnesium alloy[J].Materials Science & Engineering, A. Structural Materials: Properties, Misrostructure and Processing,2001(1/2):38-44.
[4] Jeong-Whan Han;Dong-Jin Kim;Byung-Don You .Effect of Gas Bubbling and Impeller Agitation on Degassing Kinetics during Magnesium Alloy (AZ91D) Melt Recycling-Water Model Approach[J].Materials Science Forum,2003(0):192-199.
[5] WATANABE T;HUANG Y C;KOMATSU R et al.Study on degassing treatment for molten magnesium[J].Light Metals,1976,26(06):266-272.
[6] BAKKE P;LAURITZEN J L;ENGH T A.Hydrogen in magnesium absorption,removal and measurement[J].Light Metals,1991:1015-1023.
[7] MIKUCKI B A;SHEAROUSE Ⅲ J D.The effects and removal of hydrogen gas in AZ91 alloy[J].IMA,1993:62-73.
[8] 胡中潮,张二林,曾松岩.铸造镁合金旋转喷吹除气的试验研究[J].特种铸造及有色合金,2006(03):139-141.
[9] XU Si-xiang,WU Shu-sen,MAO You-wu,AN Ping.Establishment of hydrogen measurement system for magnesium alloy melt[J].中国有色金属学会会刊(英文版),2006(z3):1677-1680.
[10] 杨长贺;曹兴言;王甲运 等.多孔吹头通Ar精炼铝合金液的生产试验研究[J].大连工学院学报,1982,21(04):125-131.
[11] 陆树逊;顾开道;郑来苏.有色铸造合金及其熔炼[M].北京:国防工业出版社,1983