对工业供应态LY12铝合金棒材的超塑性进行了研究.结果表明:该合金在温度为753 K、应变速率为3.3×10-4s-1的拉伸变形条件下,断裂延伸率为313%,应变速率敏感性指数m值约为0.33;断裂延伸率的实验值与Ghosh-Ayres公式的理论值吻合;超塑性变形的主导机制符合Langdon大晶粒模型.
参考文献
[1] | GHOSH A K;Ayres R A .On reported anomalies in relating strain-rate sensitivity (m) to ductility[J].Metallurgical and Materials Transactions,1976,A7:1589-1591. |
[2] | Langdon T G .A unified approach to grain boundary sliding in creep and superplasticity[J].Acta Metallurgica Et Materialia,1994,42(07):2437-2443. |
[3] | Langdon T G.Grain boundary sliding as a deformation process in creep and superplasticity[J].Materials Science Forum,1994:170-172,53-58. |
[4] | Langdon T G.Cavitation in high strain rate superplasticity - implications for the flow process[J].Materials Science Forum,1997:233-234,47-62. |