采用粉末冶金法成功制备出力学性能与骨匹配的开孔型多孔钛,其孔隙率分布在8.6%~35.4%之间,平均孔径随孔隙率增加而增加;抗压强度随孔隙率的增加而降低,分布在252~848 MPa之间;通过应力-应变曲线计算得到其弹性模量在7.2~9.9 GPa之间,接近人骨弹性模量.此多孔钛有望成为理想的人工骨修复材料.
参考文献
[1] | Okazak Y;Nishimura E;Nakada H;Kobayashi K .Surface analysis of Ti-15Zr-4Nb-4Ta alloy after implantation in rat tibia.[J].Biomaterials,2001(6):599-607. |
[2] | Lyle D. Zardiackas;Douglas E. Parsell;Lance D. Dillon .Structure, Metallurgy, and Mechanical Properties of a Porous Tantalum Foam[J].Journal of biomedical materials research, Part B. Applied biomaterials,2001(2):180-187. |
[3] | C.E. Wen;Y. Yamada;K. Shimojima .Compressibility of porous magnesium foam: dependency on porosity and pore size[J].Materials Letters,2004(3/4):357-360. |
[4] | 刘辉,杨冠军,于振涛,韩建业,刘春潮.生物医用多孔钛合金材料的制备[J].钛工业进展,2010(01):9-15. |
[5] | C.E. Wen;M. Mabuchi;Y. Yamada .Processing of biocompatible porous Ti and Mg[J].Scripta materialia,2001(10):1147-1153. |
[6] | Yamada Y;Shimojima K;Sakaguchi Y et al.Effects of heat treatment on compressive properties of AZ91 Mg and SG91A Al foams with open-cell structure[J].Materials Science and Engineering,2000,280A:225-228. |
[7] | C. SAN MARCHI;A. MORTENSEN .DEFORMATION OF OPEN-CELL ALUMINUM FOAM[J].Acta materialia,2001(19):3959-3969. |
[8] | Leyens C;Peters M;陈振华.钛与钛合金[M].北京:化学工业出版社,2005 |
[9] | Samuneva B;Kozhukharov V;Trapalis C et al.Sol-gel processing of titanium-containing thin coatings Part Ⅰ Preparation and structure[J].Journal of Materials Science,1993,28(09):2353-2360. |